What is Inconel® 625 สแตนเลส ?

Inconel® 625 stainless steel, with a chromium-nickel and low carbon content, is used for its outstanding corrosion resistance especially at

elevated temperatures. This alloy has similar physical properties and fabrication characteristics as Type 304 at room temperature. The unique

chemistry of Inconel® 625 increases the corrosion resistance in salt water applications and against high temperature oxidation. In the medical

field, it has served the MRI compatible market due to its high nickel content that keeps a low magnetic permeability even at high strengths.

Inconel® 625 is more expensive than 304, but is readily available.

Inconel® 625 Products Form

  • บาร์
  • Wire
  • Sheet
  • Plate
  • Forgings
  • Pipe fittings
  • Flanges
  • Seamless & Welded pipe
  • Seamless Tube & Welded tube
  • Weld Rod

Applications for Inconel® 625

Product and technology applications of Inconel 625 include:

  • Seawater components
  • Flare stacks
  • Aircraft ducting systems
  • Fabrication with Inconel 625
  • Specialized seawater equipment
  • Chemical process equipment
  • Turbine shroud rings
  • Engine thrust-reverser systems
  • Jet engine exhausts systems
  • Boiler furnaces

Equivalents of Inconel® 625

STANDARDINCONEL 625
UNSN06625
WERKSTOFF NR.2.4856
ในNiCr22Mo9Nb
BSNA 21
GOSTХН75МБТЮ
ORЭИ602
เขาNCF 625
AFNORNC22DNB4M

Chemical Composition(%) for Inconel® 625

CSiMnPSCrNiCb+TaCoMoFeAlTi
0.1 max0.5 max0.5 max0.015 max0.015 max20.0-23.058.0 นาที3.15-4.151.0 max8.0-10.05.0 max0.4 max0.4 max

Mechanical Properties

Inconel alloy 625 is a highly sought-after alloy due to its impressive mechanical properties. It has excellent fatigue strength, tensile strength, and a high degree of creep rupture under temperatures as high as 1500F. Furthermore, its stress corrosion cracking resistance and oxidation resistance make it suitable for many extreme applications. UNS N06625 also offers superior weldability and formability compared to many other similar materials – making it an ideal choice for parts that need to be deeply formed or complexly joined. All in all, Inconel 625 is an incredibly strong and versatile solution in the competitive world of metal alloys.

PROPERTY21°C204 °C316 °C427 °C538 °C649 °C760 °C871 °C
Ultimate Tensile Strength /Mpa992.9923.9910.1910.1896.3820.5537.8275.8
0.2% Yield Strength /MPa579.2455.1434.4420.6420.6413.7406.8268.9
Elongation %444542.545483459117
Coefficient of Thermal Expansion µm/m⁰C13.113.313.71414.815.315.8
Thermal Conductivity /kcal/(hr.m.°C)8.510.712.213.51516.417.919.6
Modulus of Elasticity/ MPa2.071.931.931.861.791.651.59

Physical Properties

ENSITY8.44 g/cm 3 / 0.305 lb/in 3
MELTING POINT1290 -1350 (°C) / 2350 2460 (°F)
SPECIFIC HEAT @ 70°F0.098 Btu/lb/°F
PERMEABILITY AT 200 OERSTED (15.9 KA)1.0006
CURIE TEMPERATURE-190 (°C) / < -320 (°F)
YOUNG’S MODULUS (N/MM2)205 x 10
ANNEALED871 (°C) / 1600 (°F)
QUENCHRapid Air

Corrosion Resistance

The high alloy content of INCONEL alloy 625 enables it to withstand a wide variety of severe corrosive environments. In mild environments such as the atmosphere, fresh and sea water, neutral salts, and alkaline media there is almost no attack. In more severe corrosive environments the combination of nickel and chromium provides resistance to oxidizing chemicals, whereas the high nickel and molybdenum contents supply resistance to nonoxidizing environments. The high molybdenum content also makes this alloy very resistant to pitting and crevice corrosion, and niobium acts to stabilize the alloy against sensitization during welding, thereby preventing subsequent intergranular cracking. Also, the high nickel content provides freedom from chloride ion stresscorrosion cracking.

Heat Resistance

Inconel 625 is a titanically-alloyed nickel-chromium material designed for exceptional heat resistance. It is specifically protected against crevice corrosion and attack in many acidic environments, making it uniquely suited for use in industries where increased temperatures often lead to a breakdown of standard materials. Inconel 625 has been used in marine engineering, nuclear power productions, and other applications where prolonged exposure to high temperatures can be an issue. So if you need a material that won’t fail under intensive heat, Inconel 625 is the ideal solution.

Heat Treatment

Inconel Alloy 625 has three basic heat treatments:

(1)High Solution Anneal – 2000/2200°F (1093/1204°C), air quench or faster.

(2)Low Solution Anneal – 1700/1900°F (927/1038°C), air quench or faster.

(3)Stress Relieve – 1650°F (899°C), air quench.

The time at the above temperatures depends on volume and section thickness. Strip, for example, would require shorter times than large sections. Temperatures for treatments No. 1 and 2 are generally held for 1/2 to 1 hour, 1 to 4 hours for treatment No. 3.

Treatment No. 1 is not commonly used for applications below 1500°F (816°C). It is generally used above 1500°F and where resistance to creep is important. The high solution anneal is also used to develop the maximum softness for mild processing operations such as cold rolling or drawing.

Treatment No. 2 is the used treatment and develops an optimum combination of tensile and rupture properties from ambient temperatures to 1900°F (1038°C). Ductility and toughness at cryogenic temperatures are also very good.

Treatment No. 3 is recommended for application below 1200°F (649°C) when maximum fatigue, hardness, tensile and yield strength properties are desired. Ductility and toughness at cryogenic temperatures are excellent. When a fine grain size is desired for fatigue, tensile and yield strengths up to 1500°F (816°C), treatment No. 3 is sometimes used.

Hot Forming

The hot-working temperature range for Alloy 625 is 1650–2150°F (900–1177°C). Heavy working needs to occur as close to 2150°F (1177°C) as possible, while lighter working can take place down to 1700°F (927°C).

Hot-working should occur in uniform reductions to prevent duplex grain structure

Cold Forming

Inconel Alloy 625 can be cold-formed by the standard shop fabrication practices. The alloy should be in the annealed condition. Work hardening rates are higher than the austenitic stainless steels.

Machinability

Inconel 625 is difficult to machine (class D-2). Heavy machines, sharp tools, slow speeds and deep uninterrupted cuts to remove the work hardened layer are needed.

Welding

Inconel 625 is readily welded by GMAW (MIG), GTAW (TIG), SMAW (manual) and SAW processes. Preheat, post heat and post weld heat treatment are not required. The area around the weld must be clean to prevent contamination of the weld pool. Argon shielding gas is used.

 Normal ServiceHigher StrengthBest Corrosion Resistance
Welding ElectrodeInconel WE 112N/AInco Weld WE 686CPT
Filler MetalInconel FM 625Inco Weld FM725NDURInco Weld FM 686CPT
Flux Cored WireInco Cored 625DHN/AN/A